Brick walls are strong, but they are also rigid and brittle, and they can take only a small amount of movement before they crack (1). Most bricklayers have built in a great many articulation joints, because the drawings show where they go. Yet it is easy to install one without stopping to consider what it actually does. Here I try to explain it simply, starting with old brickwork.
The issue
Cracks take many forms, but in my experience their causes fall into two broad groups. The first is age. In a very old wall, the mortar can weaken over the years and loosen of its own accord. The second is more common. A wall that carries load is under stress all the time, and when the ground moves as well, the two act together. For that reason, the cause of a crack is often more complicated than it first appears.
Many older buildings stand on shallow, fairly flexible footings of bluestone or rubble. Concrete strip footings came into use only from the early twentieth century (2). Where the soil beneath is reactive clay, it shrinks as it dries and swells when it is wet (2), so the footing, and the wall above it, moves a little with the seasons.
Those walls were laid in lime mortar, which is weaker than the bricks and more elastic than cement. This is deliberate: when cracking does occur, it shows in the mortar joints, where it is less obvious and easier to repair (3). In my view, those soft joints did part of the work that an articulation joint does today. It is also why old lime joints should not be repointed with a strong cement mortar. Cement is too hard and rigid, and the next movement may crack the bricks rather than the joints (3).
Modern brickwork is different. Cement-based mortar is much stronger and stiffer (3), and clay bricks themselves grow slightly from the day they leave the kiln, mostly in the first six months and a little more over the rest of their life (4). A footing that deflects only about 5 mm over 10 m can be enough to crack a full masonry wall that has no articulation joints (1). If the movement has nowhere to go, the wall finds its own weak point, often at an opening, and the crack zig-zags through the joints (1).
The solution
An articulation joint simply gives the wall a planned place to move. It is a vertical gap, usually 10 or 15 mm wide, that divides the wall into separate panels (1). When the soil swells or shrinks and the footing bends slightly, each panel tilts a little as a whole, and the joint opens or closes, most at the top and hardly at all at the bottom (1)(4). The crack that would otherwise have appeared in a random place becomes a straight, sealed joint in a place the designer has chosen.
A control joint does a similar job for the bricks' own growth. Corners are especially at risk, because the two walls grow towards the same point, and so a long wall often needs a joint at or near the corner (4).
As to where the joints should go, you will often hear on site that there should be one within 5 m of a corner. The accurate answer, however, is that every articulation joint should be specified by the engineer. Sometimes that means one every 2 m, and sometimes even every 1.8 m. In my view, it depends on how the load is spread through the wall. Neither the builder nor I can put our name to a joint position, and it is not decided by whether the client likes the look of it. The engineer who designs the structure decides.
For the joint to do its work, a few things matter on the day.
Keep it clean. The joint must be free of mortar. Mortar or anything else left in the gap can stop it from closing, which defeats its purpose (1).
Use a filler that compresses. Closed-cell foam or polystyrene is suitable. Cork, fibre board and semi-rigid foam do not compress enough (1).
Seal it late. Apply a flexible sealant over a backing rod, set back slightly from the face, towards the end of the job once the early movement has taken place (1).
Ties on both sides. Place wall ties on each side of the joint, no more than 300 mm from it, at twice the usual number up the height (1).
Do not move it without asking. The position is the engineer's decision. If a joint falls in an awkward spot, ask before shifting it.

Without joints, the wall picks its own place to crack. With articulation joints, each panel tilts a little and the joints take the movement. Illustration by Artvision Brickwork, movement exaggerated, not to scale.
An articulation joint is not just a gap we leave because the drawing says so. It is the place where the wall is allowed to move, so that the wall does not choose its own place to crack. In the next post, I look at what can be done once a wall has already cracked. These are, of course, only my own views. If you see things differently, I would like to hear from you.
artvisionbrickwork@gmail.com · Artvision Brickwork
Notes
Cement Concrete & Aggregates Australia, Technical Note 61: Articulated Walling (2008). https://dmyotikqn1yoq.cloudfront.net/app/uploads/2023/10/CCAA-tn61articulatedwalling.pdf
Heritage Victoria, Floods and heritage: technical notes (glossary: footings, soil reactivity). https://www.heritage.vic.gov.au/protecting-our-heritage/disasters-and-heritage/floods-and-heritage/technical-notes
Heritage Council of Victoria, Mortars: materials, mixes and methods. A guide to repointing mortar joints in older buildings (2021). https://assets.heritagecouncil.vic.gov.au/assets/MortarsTechnicalGuide-online.pdf
PGH Bricks, Technical Manual, section 1.107 Moisture Expansion, Control Joints and Articulation Joints. https://www.pghbricks.com.au/-/media/pgh-pluto/pluto/brochures/pgh-technical-document.pdf