Stains are one of the most common problems at the end of a brick job. Some are caused by the brick wash, and some start in the brick itself. This post goes with my two posts on brick wash, Brick Wash, Part 1 and Brick Wash, Part 2. Here I go through the four stains I see most often, why each one happens, and what to do about it.

The issue

The four are acid burn, poor cleaning, vanadium stain and efflorescence. The first two come from the wash. Vanadium starts in the brick, but the wash can make it much worse. Efflorescence has nothing to do with the wash; it comes from water getting into the wall. Acid burn and vanadium can look alike at first, so people often mix them up. That matters, because hydrochloric acid, the usual brick wash acid, can turn vanadium into a stain that is much harder to remove.

Why light-coloured bricks need the most care

Brick washers generally know that light-coloured bricks need extra care, and many of them use an environmentally friendly acid on light bricks instead of straight hydrochloric acid. Industry guidance also sets a lower maximum acid strength for light-coloured clay bricks: 1 part acid to 20 parts water, against 1 to 10 for other clay bricks (1).

From what I have found, there are two reasons why light bricks need more care. First, vanadium is naturally found in cream-coloured clays, and the amount can vary a great deal within one clay pit or between pits (2). The salts are usually colourless inside the brick (1). Second, any stain is easier to see on a light face (3). Acid burn can happen on darker bricks too, but it is most obvious on cream bricks (1). On a red or brown brick, a rust-coloured stain is close to the colour of the brick itself, so it hardly shows.

I have not found clear published research on the deeper chemistry, for example whether the way the bricks are fired plays a part. Our industry is small, and not much of this is written down. If you know more about this, I would be glad to learn from you.

The solution

1. Acid burn (iron oxide stain)

A yellow, orange or brown rust-like stain (1). Both the brick and the mortar sand contain iron. In my experience, many bricks have iron you can see with the naked eye. Hydrochloric acid reacts with the iron oxide in the brick and the sand, and it forms on the face of the brick as iron oxide, which is rust. It can also leach into the mortar joint (1). Some bricks have large amounts of iron oxide just below the surface, and acid stronger than 1 part to 20 can dissolve it and cause this stain (1). It usually happens when the wall was not wetted first, the acid was too strong or left on too long, or the wall was not hosed off as the work went along (1).

Acid burn (iron oxide) stain on light-coloured brickwork

Acid burn (iron oxide stain): a yellow to orange-brown, rust-like stain on light-coloured bricks. Photo: PGH Bricks & Pavers and Think Brick Australia, The Leading Practice Guide: Bricklaying and Cleaning (2024).

The best fix is not to cause it, which is what the steps in Brick Wash, Part 2 are for. Once it is there, it can be treated with a different acid, such as phosphoric acid or oxalic acid, and oxalic acid is followed by a neutraliser (1). Test a small area first.

2. Poor cleaning

Mortar smears and cement film still on the face after the wash. Usually the wash was rushed or not finished properly. The answer is to wash it again, properly. The temptation is to make the acid stronger the second time, but in my view that is the wrong answer. Guidance notes that when acid is not given enough time to work, operators tend to increase the strength, and that is one of the causes of acid burn (1).

Mortar smears on freshly laid brickwork

Mortar smears on freshly laid brickwork. Left on the face, they are what a rushed wash fails to remove. Photo: PGH Bricks & Pavers and Think Brick Australia, The Leading Practice Guide: Bricklaying and Cleaning (2024).

3. Vanadium stain

A green or yellow-green stain. The vanadium salts are already in the clay. Water soaks into the brick, dissolves the salts and carries them to the face, and when the water dries, the salts stay on the surface (3). In my experience, it shows up after the wall gets wet, for example from morning moisture, and then dries in the sun.

Vanadium stain on light-coloured bricks

Vanadium stain: a yellow-green discolouration on light-coloured bricks. Photo: PGH Bricks & Pavers and Think Brick Australia, The Leading Practice Guide: Bricklaying and Cleaning (2024).

But acid plays a part too. The stain usually becomes visible only in slightly acidic conditions, such as rain or a normal brick clean, which is why it tends to appear after the bricks are already on site (2). Guidance also says it is often brought out by hydrochloric acid that is too strong during the first clean, or by too much water (1).

For that reason, hydrochloric acid should not be used on it. It can turn vanadium black and much harder to remove, so check for vanadium and treat it before the main wash (1). It is removed with its own product. Guidance lists options such as sodium hypochlorite, caustic soda, oxalic acid followed by a neutraliser, and proprietary cleaners (1)(2). I have used one on one of our own jobs. Vanadium is not a defect in the brick, and in exposed areas it generally washes off in time (1).

Not every green stain is vanadium, though. In my experience, green staining is worst where water pours down the wall like a waterfall. Because of the building sequence, brick wash usually happens before the downpipes, the cappings on top of the brickwork and the roof flashings are finished. So when it rains, water runs straight down certain parts of the wall. When I first saw the green staining in those areas, I took it for vanadium, but I am honestly not sure. It came off with just water and a brush, so it may have been something else, such as moss or algae starting to grow on the wet brickwork. Guidance links both to water: too much water brings more vanadium salts out (1), and moss and algae are a sign of damp brickwork (4).

With a green stain, therefore, I would start with the gentlest thing: water and a soft brush. If it does not come off, then look at vanadium. Guidance makes a similar point: green staining that does not respond to the treatment for moss and algae may be due to vanadium salts (4). Either way, if it keeps coming back in the same spot, look at where the water is coming from first. Unless the water problem is fixed, the staining is likely to keep coming back (4).

4. Efflorescence (white salt)

A white, powdery and sometimes fluffy deposit on the face of the wall. Strictly speaking, it is not a stain, and it is common on new brickwork for a while (1). It has nothing to do with the brick wash. It needs three things: soluble salts, too much water getting into the wall, and that water drying out and leaving the salts on the surface (1). The salts mostly come from the mortar, especially the cement, and also from soil in contact with the wall or sea spray near the coast. The bricks themselves are not a common source (1).

The real cause, then, is water. The most common reasons are poor cappings and flashings, new brickwork left uncovered when rain stops the bricklaying, and bricks stored on the ground on site, where they soak up water and salts before they are even laid (1). It is the same water problem as the waterfall areas above. If it keeps coming back, it may be a warning that water is getting into the wall through faulty cappings, flashings or pipes (1).

Efflorescence, white salt deposits on brickwork

Efflorescence: white salt deposits on the brick face. Photo: PGH Bricks & Pavers and Think Brick Australia, The Leading Practice Guide: Bricklaying and Cleaning (2024).

Most efflorescence disappears on its own over time. To speed it up, brush it off with a stiff dry brush, and collect the salt with a dust pan or vacuum so it does not get back into the wall or the paving below. A damp cloth, wrung out well, can pick up what is left. Do not hose it off. Water just dissolves the salt back into the brick, and it comes back when the wall dries (1). And fix the water first, or the staining will keep coming back (4).

Not every white mark is efflorescence, though. A hard, milky film that disappears when the wall is wet but will not wash off with water may be a calcium stain, which can come from incorrect acid cleaning, among other things (1).

Most stains are easier to prevent than to remove. If you are not sure what a stain is, test a small area first, and check the brick manufacturer's cleaning advice before using anything strong.

These are, of course, only my own views. If you see things differently, I would like to hear from you.

artvisionbrickwork@gmail.com · Artvision Brickwork

Notes

  1. Think Brick Australia, Clay Masonry Cleaning Manual (Manual 13), published on the Littlehampton Brick website. https://littlehamptonbrick.com.au/wp-content/uploads/2024/09/manual-13-clay-masonry-cleaning-manual.pdf

  2. Midland Brick, Product Fact Sheet: Understanding Vanadium Stains (2024). https://www.midlandbrick.com.au/wp-content/uploads/2025/09/Product-Fact-Sheet-Vanadium.pdf

  3. Brick Industry Association (US), Technical Note 23, Stains: Identification and Prevention. https://www.gobrick.com/media/file/23-tn23.pdf

  4. Brickworks (New Zealand), Design Note M1: Maintenance of Bricks (October 2024). https://www.tripdocs.net/td/brickworks.co.nz/cadbim/pdf/design_notes/Brickworks%20Design%20Note%20M1%20-%20Maintenance%20Of%20Bricks.pdf